ASTM A193 Bolting
ASTM A193 is the standard for alloy steel and stainless steel bolting used in high-temperature or high-pressure service, such as the studs on flanges, valves and pressure vessels. The common grades are B7, B7M and B16 in alloy steel, and B8 and B8M in stainless steel.
A193 bolting from Eastwood
- Studs, bolts and cap screws made to the grade, class and dimensions on your drawing
- Heat treatment done in house or by outside heat treaters, to the grade's requirements
- Stainless grades passivated in house
- Material certifications with heat numbers shipped with the order
- An AS9100D and ISO 9001:2015 certified shop in Houston, Texas
A193 grades
| Grade | Material | Condition |
|---|---|---|
| B7 | Chromium-molybdenum steel (4140, 4142 or 4145) | Quenched and tempered |
| B7M | Same steel as B7 | Tempered to a lower, controlled hardness |
| B16 | Chromium-molybdenum-vanadium steel | Quenched and tempered |
| B8 Class 1 | 304 stainless | Carbide solution treated |
| B8M Class 1 | 316 stainless | Carbide solution treated |
| B8 and B8M Class 2 | 304 and 316 stainless | Solution treated and strain hardened |
Mechanical properties by grade
MPa and mm figures are conversions of the inch values, rounded. ASTM A193M lists its own metric minimums, which differ slightly.
Grade B7
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| 2-1/2 and under | 125 | 105 | 16 | 50 | 321 HBW or 35 HRC |
| Over 2-1/2 to 4 | 115 | 95 | 16 | 50 | 321 HBW or 35 HRC |
| Over 4 to 7 | 100 | 75 | 18 | 50 | 321 HBW or 35 HRC |
Grade B7M
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| 4 and under | 100 | 80 | 18 | 50 | 235 HBW or 99 HRB |
| Over 4 to 7 | 100 | 75 | 18 | 50 | 235 HBW or 99 HRB |
Grade B16
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| 2-1/2 and under | 125 | 105 | 18 | 50 | 321 HBW or 35 HRC |
| Over 2-1/2 to 4 | 110 | 95 | 17 | 45 | 321 HBW or 35 HRC |
| Over 4 to 8 | 100 | 85 | 16 | 45 | 321 HBW or 35 HRC |
Grades B8 and B8M, Class 1
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| All diameters | 75 | 30 | 30 | 50 | 223 HBW or 96 HRB |
Grade B8, Class 2
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| 3/4 and under | 125 | 100 | 12 | 35 | 321 HBW or 35 HRC |
| Over 3/4 to 1 | 115 | 80 | 15 | 35 | 321 HBW or 35 HRC |
| Over 1 to 1-1/4 | 105 | 65 | 20 | 35 | 321 HBW or 35 HRC |
| Over 1-1/4 to 1-1/2 | 100 | 50 | 28 | 45 | 321 HBW or 35 HRC |
Grade B8M, Class 2
| Diameter (in.) | Tensile, min (ksi) | Yield, min (ksi) | Elongation, min (%) | Reduction of area, min (%) | Hardness, max |
|---|---|---|---|---|---|
| 3/4 and under | 110 | 95 | 15 | 45 | 321 HBW or 35 HRC |
| Over 3/4 to 1 | 100 | 80 | 20 | 45 | 321 HBW or 35 HRC |
| Over 1 to 1-1/4 | 95 | 65 | 25 | 45 | 321 HBW or 35 HRC |
| Over 1-1/4 to 1-1/2 | 90 | 50 | 30 | 45 | 321 HBW or 35 HRC |
Class 2 strength drops as diameter goes up, because strain hardening does less on a bigger bar. Check your size in the table before you call out Class 2 on anything over 3/4 in. The Class 2 table stops at 1-1/2 in. Above that, talk to us before you put Class 2 on the drawing.
Tensile strength by diameter
Chemistry
| Element (%) | B7 | B16 | B8 (304) | B8M (316) |
|---|---|---|---|---|
| Carbon | 0.38 to 0.48 | 0.36 to 0.47 | 0.08 max | 0.08 max |
| Manganese | 0.75 to 1.00 | 0.45 to 0.70 | 2.00 max | 2.00 max |
| Phosphorus, max | 0.035 | 0.035 | 0.045 | 0.045 |
| Sulfur, max | 0.040 | 0.040 | 0.030 | 0.030 |
| Silicon | 0.15 to 0.35 | 0.15 to 0.35 | 1.00 max | 1.00 max |
| Chromium | 0.80 to 1.10 | 0.80 to 1.15 | 18.0 to 20.0 | 16.0 to 18.0 |
| Nickel | 8.0 to 11.0 | 10.0 to 14.0 | ||
| Molybdenum | 0.15 to 0.25 | 0.50 to 0.65 | 2.00 to 3.00 | |
| Vanadium | 0.25 to 0.35 | |||
| Aluminum, max | 0.015 |
These are heat analysis limits from the current edition. A product check on finished parts is allowed a small variation, 0.02 on carbon for B7, and older editions printed slightly wider ranges such as carbon 0.37 to 0.49. If a mill cert sits just outside this table, check it against the edition on your order before rejecting it.
B7M has the same chemistry as B7. The difference is in the testing: every B7M stud or bolt is hardness tested, not a sample from the lot.
Which nut goes with which stud
| A193 stud | Usual A194 nut |
|---|---|
| B7 | Grade 2H |
| B7M | Grade 2HM |
| B16 | Grade 7 |
| B8 | Grade 8 |
| B8M | Grade 8M |
See ASTM A194 nuts for hardness and proof stress by grade. A B7M stud with a 2H nut is a mistake in sour service. Match the M grades. Grade 4 nuts were once paired with B16 and were withdrawn from A194 in 2017, so Grade 7 is the pairing now.
Grade marks
Each A193 stud is stamped on one end with its grade symbol and the manufacturer's mark. On a headed bolt the marks are on the head. If the end of a stud is blank, do not assume the grade. Studs under 3/8 in. and bolts under 1/4 in. are too small to stamp, so marking on those is agreed with the buyer.
Threads
1 in. and under is normally UNC. Above that the usual callout is 8UN, eight threads per inch. If the print gives only grade and diameter, we ask before we cut.
B7, B7M or B16
B7 is the default for flange bolting. B7M is the same steel tempered to a lower strength with hardness held to 235 HBW, which is what sour-service specifications call for. B16 has vanadium added and holds its strength at a higher temperature than B7. If the joint runs hot enough that B7 relaxes, the engineer will usually have B16 on the drawing already. We quote what the print says.
Tempering and service temperature
The alloy steel grades are quenched and tempered. The standard sets a minimum tempering temperature for each one.
| Grade | Minimum tempering temperature |
|---|---|
| B7 | 1100°F (593°C) |
| B7M | 1150°F (620°C) |
| B16 | 1200°F (650°C) |
A193 does not set a service temperature. That limit comes from the design code for the joint, such as ASME B31.1, B31.3 or Section VIII. As a rough guide, B7 is the usual choice up to about 750 to 850°F, and B16 is used above that to about 1100°F. For low-temperature service the usual specification is ASTM A320, not A193.
Sour service
B7M is the A193 alloy grade used where hydrogen sulfide is present. Its hardness is held to 235 HBW, about 22 HRC, which is the limit sour-service rules work to. If your specification cites NACE MR0175 / ISO 15156 or NACE MR0103, put it on the request so the testing and paperwork are quoted with the parts.
Coatings
A193 studs ship plain unless the order calls for a coating. The common callouts are PTFE (fluoropolymer) coating, zinc plating and hot-dip galvanizing. A coated stud usually has a lower temperature rating than a plain one, so check the coating against the service temperature. Put the coating and its specification on the request and we quote it with the parts.
A193 compared
A193 sits among the bolting standards buyers most often weigh it against:
| Specification | Service | Common grade | Minimum tensile (ksi) |
|---|---|---|---|
| A193 | High temperature or high pressure | B7 | 125 to 2-1/2 in. |
| A320 | Low temperature, impact tested | L7 | 125 to 2-1/2 in. |
| A453 | High temperature, superalloy | 660 (A286) | 130 |
| A354 | General, quenched and tempered alloy | BD | 150 |
| A307 | General, carbon steel | A | 60 |
Common questions
What does ASTM A193 mean?
It is ASTM's specification for alloy steel and stainless steel bolting for high-temperature or high-pressure service. It covers bolts, studs and screws. A grade such as B7 or B8M tells you the material and the strength.
What is the difference between A193 and A194?
A193 covers the bolting: studs, bolts and screws. A194 covers the nuts that go on them. A flange set is normally ordered as A193 studs with A194 nuts in the matching grade.
Is A193 B7 stainless steel?
No. B7 is chromium-molybdenum alloy steel, quenched and tempered. It is strong and it rusts, so it is often coated or plated.
Is A193 B8 stainless steel?
Yes. B8 is 304 stainless and B8M is 316 stainless. Class 1 is solution treated. Class 2 is also strain hardened, which makes it much stronger in small diameters.
Can A193 studs be longer or larger than a distributor stocks?
Yes. That is most of what we make. Send the grade, diameter, length and thread, and we machine the studs from bar.
Sizes Eastwood makes
We machine A193 studs from bar up to 3.000 in. diameter, with small diameters on our Swiss machines. Hex bolts and cap screws are smaller, because the head sets the bar size. Larger parts are quoted too.
Related pages
All specifications · A193 Grade B7 studs · ASTM A194 nuts · ASTM A320 low-temperature bolting · ASTM A453 Grade 660 · Industrial studs · Stainless steel fasteners · Oil and gas · Chemical and refining · Quality, certifications and PPAP
Industries that use this spec: Oil and Gas · Chemical Refining · Power Generation · Marine and Naval · Water Systems
Other specification guides: ASTM F1554 anchor rods · ASTM A325 structural bolts · A193 Grade B7 · ASTM A194 nuts · ASTM A320 · ASTM A453 Grade 660 · ASTM A354 · ASTM F593 and F594 · SAE J429 Grades 5 and 8 · ASTM A574 socket head cap screws · ASTM A307 · ASTM A449 · ASTM A563 nuts · ASTM F436 washers · ASTM A490 structural bolts
Quote A193 bolting
Send the grade, class, diameter, length, thread and quantity, or send the print. Add any coating, sour-service or testing requirement and the date you need the parts. Lead time comes back with the price.
Request a quote sales@emfasteners.com
The tables summarize minimum requirements from ASTM A193/A193M. The standard itself governs. Check the current edition for your order.